1708 fiberglass cloth is a type of biaxial reinforcement, not a rival to it. The difference is one extra layer. A 1708 combines a ±45° biaxial fabric with a stitched chopped strand mat, while a plain biaxial is that same ±45° fabric on its own. Choose 1708 when you want shear strength and quick thickness build in one pass. Choose a plain biaxial when you need to control weight, angle or thickness yourself. Choose a woven 0/90 fabric when drape, surface finish or repairs matter more than torsion.
This guide compares 1708 and biaxial fiberglass cloth in detail, uses woven fabric only as a supporting comparison, says which one fits which job and why, and ends with a buying guide.
What 1708 Is and Why It Is Built That Way

The 1708 name describes a two-layer build. The first layer is 17 oz per square yard of ±45° biaxial fabric. The second is a chopped strand mat at 0.75 oz per square foot. The two are held together by stitching, with no chemical binder joining them.
Each part has a reason behind it:
- ±45° fibers are aligned with the directions twisting and shear loads act. This counters the twisting forces that standard 0°/90° weaves handle poorly.
- Non-crimp fibers lie flat instead of bending over and under each other, so load transfers sooner.
- The stitched mat layer creates flow paths for resin, which speeds saturation in hand lay-up and vacuum infusion.
- Epoxy, polyester and vinyl ester are all compatible.
These are design reasons, not guaranteed results. How a finished part performs also depends on the resin system, the lay-up design (layer count, sequence and fiber content) and the manufacturing process, whether hand lay-up or infusion. For context, the ASTM D3518 test method measures in-plane shear response by tension testing a ±45° laminate, which is why ±45° fibers are the standard way to carry shear. The resin flow benefit of the mat layer depends on resin viscosity and the process, so treat the supplier’s data as a starting point and confirm both effects with a test panel in your own resin and process.
It comes in three grades. Standard E-glass suits boat hulls, automotive panels and sports gear. ECR-glass has a boron-free structure that resists acid leaching and alkaline attack, which suits chemical tanks and scrubbers. Fine-surface adds an ultra-thin tissue to prevent print-through on high-gloss parts. The mat weight can also change: 1705 (0.5 oz mat) for thinner profiles, and 1715 (1.5 oz mat) for impact resistance and larger resin interlaminar zones.
Suppliers describe this stitched mat construction as a mat, a cloth or a combo. Specify it by construction, not by name.
What a Plain Biaxial Offers Instead

A biaxial fiberglass cloth is the ±45° fabric without the mat. The regular angle is ±45°, and it can be adjusted from +30° to +80°. Total weight runs from 300 to 1200 g/m², and the maximum width reaches 101 inches. It is a multiaxial, non-curling reinforcement with layers sewn together by polyester yarn, used in wind energy, shipbuilding, molds, automotive, aviation and defense.
Why choose it: you control the build. If your laminate designer specifies a particular weight or angle, or wants separate mat layers placed in specific positions, a plain biaxial gives that freedom. It also avoids paying for and laminating a mat layer you do not need.
Where Woven 0/90 Fabric Still Wins
Woven fabric is the supporting comparison here. It fits jobs where torsion is not the main load, such as surface layers, repairs and small parts, and tightly curved shapes. A 0/90 fabric can be rotated to 45°, but you cut, place and rotate each layer, whereas stitched biaxial gives you that fiber direction in one pass. The choice of weight and weave for those jobs is a separate decision from choosing between 1708 and a plain biaxial, so this guide does not go into it.
The Short Answer in One Table
Feature | 1708 | Plain Biaxial | Woven 0/90 |
| Construction | ±45° fabric stitched to chopped strand mat | ±45° fabric sewn with polyester yarn | Plain, twill or satin weave |
| Fiber direction | ±45° plus random mat | ±45°, adjustable from +30° to +80° | 0° and 90° |
| Mat layer | Built in | None | None |
| Typical weight | 17 oz/sq yd biaxial plus mat | 300-1200 g/m² total | 4 oz, 6 oz and 10 oz are the most used |
| Strongest at | Twist and shear, fast thickness build | Twist and shear, with tailored weight and angle | Surface finish, drape, repairs |
Which To Choose: By Application
The right reinforcement depends on what the part has to survive, so each application below is worked through the specifications that change the result: fiber angle, weight, mat layer, glass type, width and resin.
Boat hulls, transoms and stringers

These parts twist and slam against waves, so the ±45° fibers of 1708 fiberglass cloth are lined up with the load that does the damage. The mat face builds thickness quickly, which matters when heavy sections are laminated and every extra pass costs labor hours. Standard E-glass is the grade that suits general hull work, and the standard 0.75 oz mat is the right starting point for most hulls and transoms. Move to 1715 when a panel is likely to take impacts, because the 1.5 oz mat gives a larger resin interlaminar zone.
Stringers are usually wrapped with narrow tapes, so slit width matters. Slitting runs from 4 to 100 inches with locked-edge stitching, so tapes stay intact on vertical and overhead lay-ups. Order widths that match the mold and stringer geometry rather than trimming wide rolls down. For boat building, the related fiberglass mat for boats range is worth reviewing too. Polyester, vinyl ester and epoxy are all compatible, but your own system should be proven on a test panel.
Wind blade skins and roots
A blade shell acts as a torsion box, so shear carried by ±45° glass is central to the design. A US Department of Energy project appendix on blade fabrics lists an E-BXM 1708 ±45° mat fabric among those modeled, and notes that double-bias fabrics cover most of the skin area of the CX-100 test blade.
Whether to buy 1708 or a plain biaxial depends on how the laminate designer wants the build laid out. If the schedule calls for mat in specific positions, or a fiber angle other than ±45°, the plain biaxial is the better fit, since its angle can be adjusted from +30° to +80° and its total weight set anywhere from 300 to 1200 g/m². If the schedule is built around the stitched mat construction, 1708 fiberglass cloth saves a layer and a pass.
Fatigue is the concern either way. NREL fatigue testing of laminates with 0° and ±45° layers found fatigue resistance varied with fiber content and the share of ±45° reinforcement, and was poorer than expected at high fiber contents and high ±45° proportions. Those are results for specific test laminates, so they will not transfer exactly to another layup. They are a reason to settle the ±45° share with the designer and not push it higher on the assumption that more is safer. Widths up to 101 inches on the plain biaxial are worth matching to the shell geometry as well.
Chemical tanks and scrubbers

Here the glass type decides how long the structure keeps its strength. Standard E-glass can be embrittled by acid or alkali, so the ECR grade of 1708 fiberglass cloth, with its boron-free structure, is the grade for chemical storage tanks, flue gas desulfurization units and scrubbers. Have the grade written on the datasheet, because a verbal confirmation is not much to rely on if a vessel fails years later. The resin has to resist the same chemicals, since the glass is only half of the barrier, so give your resin supplier the chemical list, concentrations and operating temperatures before you fix the reinforcement.
Master molds and show faces
A master mold or a visible, high-gloss surface will show any fiber texture sitting just under the finish. Fine-surface 1708 solves that with an ultra-thin tissue on the face, which prevents print-through. Request a sample panel and look at it under raking light before committing to volume. If the face layer is only a thin skin over something else, a 4 oz woven cloth is the alternative, since it is thick enough to stop the print of heavy fabrics underneath from showing through.
Thin laminates and custom weight or angle
When the part is thin, the mat layer of 1708 fiberglass cloth can add thickness you cannot afford. Two routes exist. The first is 1705, with its lighter 0.5 oz mat, which keeps the stitched construction and trims the build. The second is a plain biaxial, which removes the mat entirely and lets you set the thickness through total weight, anywhere from 300 to 1200 g/m². Pick the plain biaxial if you also need a different fiber angle, or if you want to place chopped strand mat in specific positions yourself.
Surface layers, small repairs and tight curves

Woven cloth is the supporting option when torsion is not the main load. For surface layers, repairs and tight curves, drape and a clean finish matter more than shear strength, and a satin weave follows curved surfaces best. Weight and weave for these jobs are a separate decision from choosing between 1708 and plain biaxial.
Parts loaded mainly in bending
A ±45° layer carries shear, not everything. If the part bends along one axis, neither 1708 nor a plain biaxial is the whole answer, and 0° reinforcement needs to be added. The balance between 0° and ±45° layers belongs with your laminate designer, as the NREL results above suggest.
How To Choose Your Specification
Specification choices stack on each other, so work through them in this order. Each answer limits the next, and the same sequence applies to any laminate reinforcement.
- The dominant load comes first: If the part twists or takes shear, you are choosing between 1708 and a plain biaxial. If it mostly bends, you need 0° layers as well, and the choice of biaxial becomes secondary. If torsion is minor and the priority is a clean surface or a repair, you are in woven territory. Answering this before buying avoids a good product ending up in the wrong laminate.
- Fiber angle decides between 1708 and plain biaxial: The 1708 is ±45°. A plain biaxial is regularly ±45° but can be adjusted from +30° to +80°. If your laminate schedule specifies a different angle, only the plain biaxial can meet it.
- Weight and thickness control the laminate build: In a 1708 the biaxial layer is fixed at 17 oz per square yard, so you tune the build through the mat option. A plain biaxial gives total weight from 300 to 1200 g/m², which lets you set thickness directly. Matching weight to the thickness budget avoids both over-building and a laminate that is too thin to do its job.
- The mat layer is a thickness and impact decision: The standard 0.75 oz mat suits general work. The 1705, with a 0.5 oz mat, suits thinner profiles. The 1715, with a 1.5 oz mat, suits parts where impact resistance and a larger resin interlaminar zone matter. Do not use price to choose between them, because a cheaper roll that forces a redesign is not cheaper in the end.
- Glass type follows the environment: Standard E-glass for general work in hulls, panels and sports gear, ECR for acid or alkaline exposure, and fine-surface where the face will be seen on a gloss finish.
- Construction type affects how the layers behave: In 1708 and plain biaxial, layers are held by stitching, with no chemical binder in the 1708, so there is no binder for the resin to attack. The stitching thread and your resin system should still be checked together.
- Resin and process come next: Epoxy, polyester and vinyl ester are all compatible, and the resin ratio must be controlled well before applying. Whether you laminate by hand or by vacuum infusion changes how much the mat layer helps. The mat is meant to create flow paths, so both processes can benefit, but the effect depends on the resin and the lay-up, and the only reliable proof is your own test panel.
- Width and roll format cut waste: The 1708 is slit from 4 to 100 inches with locked-edge stitching. A plain biaxial reaches 101 inches in maximum width. Waste depends on how closely the roll width matches the part. For example, cutting a 30 inch tape from a 40 inch roll leaves 10 of 40 inches as offcut, which is 25%, while a roll slit to 30 inches leaves only the edge trim. Your saving is the difference between those two figures, so calculate it from your own tape widths and quantities before counting on any percentage.
The layer count belongs to your laminate designer. It should not be guessed from the product name, the weight or the quote.
| Specification | Options | Where it makes the difference |
|---|---|---|
| Fiber angle | ±45° (1708), ±45° adjustable +30° to +80° (plain biaxial) | Parts with non-standard load directions |
| Total weight | Fixed biaxial plus mat (1708), 300-1200 g/m² (plain biaxial) | Thin laminates and tailored builds |
| Mat layer | 1705, 1708, 1715 | Thickness, impact resistance, interlaminar zone |
| Glass type | Standard E-glass, ECR, fine-surface | Chemical service, show faces |
| Width | 4-100 in (1708), up to 101 in (plain biaxial) | Waste and tape handling |
| Resin and process | Epoxy, polyester, vinyl ester; hand lay-up or infusion | Wet-out and bonding |
For help matching 1708 fiberglass cloth or a plain biaxial to your laminate schedule, send ZS Fiberglass your load case, resin and widths, and ask for a sample before committing to volume.
FAQs
1.Is 1708 the Same as Biaxial Fiberglass Cloth?
No. 1708 is a biaxial fabric stitched to a chopped strand mat. A plain biaxial fiberglass cloth is the ±45° fabric without the mat.
2.Do I Need the Mat Layer?
Choose it when you want quick thickness build and better resin flow in one pass. Skip it when the laminate is thin or you want to place mat layers separately.
3.Can I Use Woven Cloth Rotated to 45° Instead?
It can be done, and 10 oz cloth is used that way in boat and mold building. You cut and rotate each layer, whereas stitched biaxial gives the fiber direction in one layer.
4.Which Grade of 1708 Should I Choose?
Standard E-glass for hulls, panels and sports gear, ECR for acid or alkali exposure, fine-surface for gloss finishes.
5.How Should I Approve a Sample?
Check weight, width and stitching against the datasheet, then laminate a test panel and inspect wet-out, voids and edge stability.
6.Which Resins Work?
Polyester, vinyl ester and epoxy all work with both products, and the resin ratio must be controlled well before applying.